Ferromagnetic thin film and spin current (5) -Angular dependence (1) -

ER190006E

The spectra of ferromagnetic resonance (FMR) usually drastically change its resonant field relative to the applied magnetic field. This is due to the demagnetizing field term originating from the anisotropy of samples. Measurement of the dependence of FMR on angular position relative to the applied magnetic field makes it possible to get information about magnetic parameters of samples (e.g. saturation magnetization, 4πMS) and to correctly elucidate the angular dependence of the inverse spin-Hall effect.

Sample and method

FMR spectra were measured with the step size of 15 degree against the applied magnetic field using the angular rotation device (ES-UCR3X in Fig. 1). The sample was the same metallic bilayer thin film reported on JEOL application note[1].

Fig. 1 ES-UCR3X (Angular rotation device).

The angular dependence of FMR spectra

The magnetic parameters were estimated as 4πMS = 0.344 T、(ω/γ) = 0.32 T using the experimental results as shown in Fig. 2 (a) and the equation (2). Furthermore, it can be possible to calculate the relationship θH with θM, using the equilibrium condition expressed in eq. (1), as shown in Fig. 2 (b)[2, 3].

1829_01_01

Substituting the four parameters to the resonant condition expressed in eq. (2), allows the resonant fields can be calculated[2, 3]. The result of simulation which Fig. 2 (a) shows matches the obtained experimental data very well.

Fig. 2 an experimental result and analysis of the angular dependence of FMR spectra.

References

[1] JEOL RESONANCE Inc. Application note No. ER190002
[2] K. Ando, Y. Kajiwara, S. Takahashi, S. Maekawa, K. Takemoto, M. Takatsu, and E. Saitoh, Phys. Rev. B, 78(2008) , 014413.
[3] K. Ando, S. Takahashi, J. Ieda, Y. Kajiwara, H. Nakayama, T. Yoshino, K. Harii, Y. Fujikawa, M. Matsuo, S. Maekawa, and E. Saitoh, J. Appl. Phys. 109(2011), 103913 .

Please see the PDF file for the additional information.
Another window opens when you click.

PDF 313KB

SEARCH APPLICATIONS

Close
Notice

Are you a medical professional or personnel engaged in medical care?

Yes

No

Please be reminded that these pages are not intended to provide the general public with information about the products.

JEOL Instrument Basics

Easy explanation about mechanisms and
applications of JEOL products

Contacts

JEOL provides a variety of support services to ensure that our customers can use our products with peace of mind.
Please feel free to contact us.