Fraction base KMD plots for a high molecular weight poly(3-hydroxybutyrate) polyester following its on-plate alkaline degradation and SpiralTOF™ analysis"

MSTips No. 283

Introduction: mathematical background

High molecular weight polymers are often MS-silent due to their inherent high dispersity (ĐM) or detected in the high mass range with low resolving power. An "on-plate" alkaline degradation has thus been developed as a sample pre-treatment on the MALDI target with tenths of ng of polymer to cut long industrial polyester chains into short oligomers amenable to MALDI-HRMS [1]. The complicated mass spectrum of P3HB oligomers was analyzed by fraction base Kendrick mass defect (KMD) plot [2]. Fraction base KMD analysis has been developed from the regular KMD analysis to modify the aspect and separation capabilities of the KMD plots depending on a divisor (noted X) in addition to the base unit (noted R) via a fraction base R/X [3].

Fig. 1. Calculation methods of fraction base KMD.

Experimental

Poly(3-hydroxybutyrate) (P3HB, Mn = 2.6 × 105 g mol-1, ĐM=2.7) was from Sigma-Aldrich (St. Louis, MO,USA). All other chemicals and solvents were from FUJIFILM Wako Pure Chemical Corporation (Osaka, Japan) unless otherwise mentioned. 1 μL of P3HB in THF at 1 mg mL-1 was drop-casted on a disposable MALDI target plate (Hudson Surface Technology, New Jersey, USA) to form a polymer thin layer. 1 μL of sodium hydroxide in methanol (10 mg mL-1) was deposited on the sample layer and left to air-dry for 5 min. The excess amount of alkaline reagent was washed with distilled water. After drying, 1 μL of 2,4,6-trihydroxyacetophenone (THAP, Protea Biosciences, West Virginia, USA) in THF (20 mg mL-1) was applied on the sample spot as matrix. Mass spectra were recorded with a JMS-S3000 SpiralTOF™ mass spectrometer. Plots were computed using msRepeatFinder 3.0 from the peak list exported using msTornado™.

MALDI mass analysis

Intense ion series of P3HB oligomers are observed in MALDI-MS (Fig. 1A). Six main series varying by their end-groups are detected (Fig. 1B) but assigning and visualizing all congeners remains time-consuming and poorly intuitive.

Fig. 1. (A) MALDI SpiralTOF mass spectrum of a high molecular weight P3HB following its on-plate degradation (inset: zoom shot with assignments). (B) P3HB ion series noted I-VI

Fig. 1. (A) MALDI SpiralTOF mass spectrum of a high molecular weight P3HB following its on-plate degradation (inset: zoom shot with assignments). (B) P3HB ion series noted I-VI.

Regular and resolution-enhanced KMD plots

The regular KMD plot computed from the MALDI mass spectrum displays a cloud of points aligned horizontally (Fig. 2A). Zooming in is mandatory as the points are clustered within a restricted portion of the plot due to a very limited change of KMD with the variation of isotope or end-group composition [4]. Two poorly resolved groups of points are seen (Fig. 2B) while six series are expected considering the mass spectral data.

Fig. 2. Full-scale regular KMD plot from the mass spectrum of P3HB with C4H6O2 as base unit using msRepeatFinder.

Fig. 2. Full-scale regular KMD plot from the mass spectrum of P3HB with C4H6O2 as base unit using msRepeatFinder.

Activating the "Fraction Base KMD" option in msRepeatFinder and decreasing the value of X from 86 (regular KMD plot) to 85, the resolution-enhanced KMD plot greatly separates the six P3HB series at full scale thanks to a greater variation of KMD by the change of composition (Fig. 3A). Decreasing X of one unit at X=84, the resolution-enhanced KMD plot additionally resolves the isotopic patterns (1st line: 12C, 2nd line: 13C1, …) and discriminates the six series even better (Fig. 3B, X=84).

Fig. 3. Full scale fraction base KMD plots computed with the fractional base units (A) 3HB/85 and (B) 3HB/84 using msRepeatFinder.

Fig. 3. Full scale fraction base KMD plots computed with the fractional base units (A) 3HB/85 and (B) 3HB/84 using msRepeatFinder.

Grouping mode with the resolution-enhanced KMD plot

The "grouping mode" in msRepeatFinder combined with the fraction base KMD analysis allows each ion series to be labelled in the mass spectrum and the plot with visual color coding via a simple selection of points (Fig. 4). The high separating power reached with 3HB/84 further allows the selection of monoisotopic peaks (12C, light green dots) from the main series I (dark green dots). Unselected ion series can also be hidden to further help at visualizing the polymeric series from the background peaks.

Fig. 4. (A) Fraction base KMD plot computed with the fractional base unit 3HB/84 in grouping mode to label the series in the mass spectrum (B).

Fig. 4. (A) Fraction base KMD plot computed with the fractional base unit 3HB/84 in grouping mode to label the series in the mass spectrum (B).

Conclusions

The KMD analysis becomes dynamic with the introduction of the "Fraction Base KMD" relying on the resolution-enhanced methodology. It is a highly versatile tool as decreasing or increasing the value of the fraction leads to numerous favorable separations of ion series varying by their isotopic composition, end-groups or adducted ion. It can be successfully adapted to any type of homopolymers and any type of mass spectral data of medium to ultrahigh accuracy.

Acknowledgements

This application note is written based on the results of a joint research project with Sayaka Nakamura, Thierry Fouquet and Hiroaki Sato from the Research Institute for Sustainable Chemistry, National Institute of Advanced Industrial Science and Technology (AIST).

References

[1] S. Nakamura, T. Fouquet, H. Sato. J. Am. Soc. Mass Spectrom. 2019, 30, 355.
[2] H. Sato, S. Nakamura, K. Teramoto, T. Sato. J. Am. Soc. Mass Spectrom. 2014, 25, 1346.
[3] T. Fouquet, H. Sato. Anal. Chem. 2017, 89, 2682.
[4] S. Nakamura, R. B. Cody, H. Sato, T. Fouquet. Anal Chem. 2019, 91, 2004.

If you want to see a printed version, please click this PDF file.

PDF 845KMB

Related Products

Solutions by field

Close
Notice

Are you a medical professional or personnel engaged in medical care?

Yes

No

Please be reminded that these pages are not intended to provide the general public with information about the products.

JEOL Instrument Basics

Easy explanation about mechanisms and
applications of JEOL products

Contacts

JEOL provides a variety of support services to ensure that our customers can use our products with peace of mind.
Please feel free to contact us.